EN 499                           E -42 6 B 32 H 5

DIN 8529                        E SY 42 76 Mn B

AWS/ASME SFA-5.1      E 7016-1-H8

 

Application / Properties: Basic low hydrogen electrode that produce crack-free and tough weld joints in as weld and heat treated condition weld meal toughness in CTOD test at -100C is very good. This electrode has smooth and clean weld blending into base metal without undercut. It is specially suited for root pass and positional welding.

Weld metal analysis in % (typical values):

C Mn Si S P  
0.06 1.50 0.30

0.02>

0.02>

 

 

Mechanical Properties of all-weld metal :

 

Yield Strength

(N/mm2)

Tensile Strength

(N/mm2)

Elongation

A5(%)

ISO-V Impact energy (j)

        +200C         -600C

Heat treatment       

 

550-640

550-640

>420

>420

>22

>22

200               80

170              60

AW

SR

 

 

AW: as-welding

SR: Stress-relived 15h/5800C

Amperage:  
Amperage (A) L (mm) Ǿ (mm)  
65-95 350 2.5  
90-140 450 3.25  
140-185 450 4  
180-240 450 5  

Materials:

Unalloyed Structural steels

St 33 to St52-3

St50-2, St60-2, St70-2

Boiler plates

H l,H ll, 17 Mn 4 

Pipe steels Inclouding corresponding TM grades

 

To St52.4

St35.8 to St45.8

StE 240-7 to StE 360-7

Fine grain structural steels

StE 255, StE 285, StE 315, StE 355   

WStE 255, WStE 285,WStE 315,WStE 355

Cryogenic Steels

TTST 35 Nu.V

Shipbuilding steels

 A,B,D,E

cast steels

GS-38 toGs-52   

 

 

Welding positions: All position

 

Redrying : required at 300°C to 350°C for 2hrs.

 

Approval: DNV