1398 N

 

Download this page As [PDF] 

EN 499                      E 46 61 Ni B 42 H5

DIN 8529                 E  SY 42 76 Ni B H5

AWS/ASME SFA-5.5            E 7018-G-H4

 

Application / Properties: Electrode for producing crack-free and tough welded joints. Weld metal is extremely metallurgical purity having a very low hydrogen content. Owing to its double covering (up to 3.25 mm SǾ), the electrode gas a stable and concentrated arc, thus being well suited or positional welding. Welds are of X-ray quality. CTOD-tested for offshore application.

 

Weld metal analysis in %(Typical values):

C Mn Si Ni S P  
0.06 1.20 0.30

0.95

<0.015

<0.015

 

 

Mechanical Properties of all-weld metal (Single values are typical values):

 

 

Yield Strength

(N/mm2)

Tensile Strength

(N/mm2)

Elongation

A5(%)

ISO-V Impact energy (j)

+200C      -600

 

AW

SR

>460

>420

530-680

500-640

>22

>25

190              70

190              60

 

 

AW: as welded

SR: stress - relieved 15hrs./580C

 

Diffusible hydrogen content (DIN 8572): HD≤5 ml/100g

Amperage:  
2.5Ǿ 3.25 Ǿ 4.0Ǿ 5.0Ǿ 6.0Ǿ  
65-95 90-140 140-185 180-250 210-310  

Materials:

Unalloyed structural steels

St33 to St 52.3, St 50.2,St 60.2, St 70.2

boiler plates

Hl,Hll ,17Mn4, 19 Mn5

pipe steels

to ST 52.4, St 35.8 to 17 Mn4, StE 210.7 to StE 415.7

Inclouding corresponding, TM-grades

Fine grain structural steels

StE 255 to StE 460, WStE 255 to WStE 460

EStE 255 to EStE 460, 15 MnNi 63

Shipbuilding Steels

 A,B,D,E

Cast steels

   Gs-38 to GS-52

 

 

 

Rebaking : required at 300°C to 350°C for 2hrs.